CHAPTER VI.

CHEMICAL AND MECHANICAL TESTS.

These tests may be necessary to confirm an optical determination or to

assist in the differentiation of the closely related species of a group,

as for example, the different plagioclases in the feldspar group. They

may also be useful in the case of opaque substances.

The ordinary chemical methods employed in mineral analyses are often not

applicable, on account of the minute size of the mineral under

investigation and the lack of sharpness in the reactions. Those

methods[132] are to be preferred which produce crystallizations

independent of the relative proportions of the materials taking part in

the reaction and also of the physical conditions invoked.

The tests can be made either on the crystal in a rock section or on the

isolated crystal or fragment, the latter method being preferable when

possible.

CHEMICAL TESTS MADE ON CRYSTAL IN SECTION.

The part of the section to be tested must be prepared by thorough

washing with alcohol and benzole to remove all traces of balsam. If the

section is covered, the cover-glass can be cut across with a diamond,

and, after heating, the desired portion removed with a knife edge. Any

portion of a section can be isolated by surrounding it with a rim of

viscous balsam or by putting on a new cover-glass, in which a small hole

has been made.[133] This hole can be accurately adjusted over the

special portion of the section and the balsam removed by alcohol and

benzole.

The treatment of rock sections with ordinary acids, such as

hydrochloric, may show the presence of easily soluble minerals[134] and

carbonates, or distinguish silicates that are soluble with jelly, or

produce etched figures on the minerals.

_Test for Carbonates._ When only present in very minute grains the test

can be made as follows: Cover the rock section with a drop of water and

a cover-glass, then allow a drop of acid to slowly diffuse through the

water film. The glass cover will prevent the escape of the gas

bubbles[135] which will thus surely be detected.

If necessary the section can be warmed by heating the projecting part of

a suitable stand, placed under the section on the stage of the

microscope.

_Test for Gelatinizing Silica._ Cover the carefully cleansed section

with a little dilute acid (commonly hydrochloric) and let stand. If too

much acid is used the resultant gelatin will spread over the whole

section and not appear simply on the gelatinizing silicate. Warm the

section, if necessary, and finally rinse off the remaining acid

thoroughly with water. Do not allow the action of the acid to continue

too long, as it is desirable to obtain only a very thin film of

gelatinous silica over the minerals attacked, so that the optical tests

can still be made on these minerals. If after the first trial the action

has not been pronounced enough, the test should be repeated.

The transparent film of gelatinous silica is made more visible by

covering the section with a drop of water, containing a dilute solution

of fuchsine. After standing for some time the section should be washed,

when only those portions covered by the gelatinous film will show the

color stain.

ETCHED FIGURES.[136]

The results of etching tests can not be regarded as very satisfactory in

the case of sections of minerals in rock sections, on account of doubt

as to the crystallographic orientation of these sections.

The symmetry of the etched figures depends essentially on the relation

of the crystal faces on which they are obtained to the planes of

symmetry.

The forms of the etched figures differ on the same face of a mineral,

depending on the reagent used, but their degree of symmetry is

independent of the reagent or its degree of concentration. The sharpest

figures are produced on crystal and cleavage faces, the figures being

less perfect on artificially prepared faces, even when polished. The

etching tests may, however, be tried to prove the presence of twinning,

or to distinguish between minerals of similar appearance but belonging

to different systems.[137]

Various acids or alkalies are used to produce the etched figures,

depending on the mineral to be tested. Different factors influence the

formation of good etched figures, and that method must be used which

seems to give most satisfactory results in the given case. The action of

the reagent should be sufficiently pronounced to develop clearly the

etched figures; at the same time the tests must be stopped before the

solvent action has been too powerful.[138] After treatment for etching

the section should be thoroughly washed and examined in some fluid of

weak refraction (with _n_ lower than that of the crystal section), such

as water or air.[139] The objective, of course, must be focused on the

surface of the section.

HEATING SECTIONS TO REDNESS.[140]

The part of the section to be tested must be removed from the object

glass, carefully cleansed of balsam, and held on platinum foil in the

oxidizing blowpipe flame. After the test the fragment used may be

remounted in Canada balsam for study.

As a result of heating:

Colorless, hydrous minerals (zeolites and chlorites) become cloudy in

appearance.

Colorless silicates, containing protoxide of iron (as olivine, or

faintly colored pyroxene or amphibole), become red or reddish-brown.

Colored minerals may change their color, chloritic substances becoming

brown or black if heated enough.

Hornblende always becomes pleochroic, and olivine sometimes becomes so.

Members of the sodalite group may be turned blue, if not already of that

color.

The dichroism (yellow to blue) of almost colorless iolite may be

developed.

Carbonaceous particles may be distinguished from the iron oxides by

being consumed.[141]

METHODS OF ISOLATING CRYSTALS OR MINERAL FRAGMENTS FOR TESTING.[142]

For the application of these methods the rock or aggregate of minerals

should be reduced to homogeneous[143] grains of uniform size (preferably

crystals or cleavages) and not to powder. This is best done by pounding

in a metal mortar, avoiding all grinding motion.

The separations required may be made by specific gravity solutions or

magnetic methods, alone or combined; and in some cases may be assisted

by chemical action.

When other methods fail it may be necessary to separate single grains

from a mixture by hand. A grooved piece of plate-glass, passed beneath

the objective of the microscope, will be found useful. The desired

grains in this groove can be picked out by means of a piece of fine

waxed thread or a fine pointed stick moistened at the end.

The _hardness_ of the homogeneous grains may be obtained by pressing

them firmly into the end of a lead stamp or holder and trying the effect

of scratching upon the faces of minerals of known hardness.

_Specific Gravity Separation._[144] Accomplished by use of fluids of

different specific gravity. These fluids can be made specifically

lighter by dilution, and hence the fragments will fall to the bottom in

order of decreasing density. Dilution of the heavy solutions to any

specific gravity may be affected empirically until the solution will

just suspend a fragment of a mineral having the desired specific

gravity; or the exact specific gravity of the solution may be determined

by the Westphal balance.

The following _indicators_ may be employed to determine the limits of

the specific gravity of the solution to be used for separation purposes

(V. Goldschmidt):

NO. NAME. LOCALITY. SP. GR.

1. Sulphur, Girgenti, 2.070

2. Hyalite, Waltsch, 2.160

3. Opal, Scheiba, 2.212

4. Natrolite, Brevig, 2.246

5. Pitchstone, Meissen, 2.284

6. Obsidian, Lipari, 2.362

7. Pearlite, Hungary, 2.397

8. Leucite, Vesuvius, 2.465

9. Adularia, St. Gotthard, 2.570

10. Elæolite, Brevig, 2.617

11. Quartz, Middleville, 2.650

12. Labradorite, Labrador, 2.689

13. Calcite, Rabenstein, 2.715

14. Dolomite, Muhrwinkel, 2.733

15. Dolomite, Rauris, 2.868

16. Prehnite, Kilpatrick, 2.916

17. Aragonite, Bilin, 2.933

18. Actinolite, Zillerthal, 3.020

19. Andalusite, Bodenmais, 3.125

20. Apatite, Ehrenfriedersdorf, 3.180

Among the heavy solutions employed may be mentioned:

Thoulet’s solution of potassium-mercuric iodide (KI: HgI_{2} = 1: 1.24),

maximum specific gravity 3.196. Klein’s solution of cadmium

borotungstate (2H_{2}O, 2CdO, B_{2}O_{3}, 9WoO_{3} + 16H_{2}O), maximum

specific gravity 3.6. These two solutions can be mixed with water in any

proportion without being decomposed. Solution of barium mercuric iodide,

maximum specific gravity, 3.588, cannot be diluted with water. Methylene

iodide (CH_{2}I_{2}), specific gravity 3.3243 at 16° C. varying with the

temperature, can be diluted with benzole but not with water.

Nitrates of silver and thallium[145] (AgNO_{3}: TlNO_{3} = 1.1) fuse at

about 75° C. to a clear mobile liquid with specific gravity over 4.5.

Can be mixed while melted with water in all proportions; but cannot be

used for separation of sulphides, as these nitrates are attacked by

them.

Possible chemical action between the minerals and heavy solutions must

not be overlooked in this method of separation.

The funnel-shaped apparatus for these separations must be so arranged,

with stop-cocks, etc., that the heavier material collected at the bottom

can be easily drawn off or removed at any stage of dilution.

These separations, for various reasons, are not always complete, but the

best results are obtained when the processes are repeated several times.

_Electro-magnetic Separation._ All iron-bearing minerals may be

separated from those free from iron by an electro-magnet.

The factors influencing the attraction of a mineral by an electro-magnet

are not definitely known, and do not seem to depend only on the

percentage of iron.

Minerals, such as amphibole, pyroxene, epidote, olivine and garnet

(containing iron), may often be separated by an electro-magnet by

regulating its magnetic intensity.[146]

_Separation by Chemical Means._ Very many different methods may be used,

depending on the nature of the work to be accomplished; but they are

generally only reliable in the hands of a good chemist. The material

should be in the state of fine powder.

As an example may be mentioned the treatment with pure concentrated HFl,

by which the minerals of a rock are attacked in a certain sequence, the

feldspars and related minerals first, then the quartz and finally the

ferro-magnesium silicates, such as amphibole, pyroxene, olivine, etc.

MICRO-CHEMICAL REACTIONS.

The first requisite is to bring the substance to be investigated into

solution. This can be done in the case of non-silicates by the ordinary

solvents, while silicates can be decomposed and investigated either by

the methods of Borichy or Behrens. Both methods rest upon the

recognition of the forms, etc., of artificially produced crystals.

The size of a fragment for testing may vary, according to circumstances,

from that of a poppy seed to a pin head. Good results are recorded from

fragments of not more than 0.2–0.7 sq. mm.

The substance to be tested is placed on glass, protected by a film of

balsam, and covered with a spherical drop of the solvent,[147] which

should be allowed to act until all the different elements composing the

sample are in solution (in the case of a very small fragment until it

has all dissolved). Transfer the solution to another protected object

glass, and, after evaporation, the crystallizations characteristic of

the different elements will be seen.

If the evaporation is too rapid and the crystallizations incomplete, the

residue should be redissolved in water, or a very dilute solution of the

solvent employed, transferred to a fresh glass and allowed to

recrystallize.

Borichy’s Method.[148] (Hydrofluosilicic Acid.)

This method has the advantage of simplicity of manipulation and relative

distinctness in results; but on the other hand these results are only

obtained after several hours, and the temperature has an influence on

the crystalline forms obtained. It is well to make the tests in a

temperature of about 15° C.

Put a spherical drop of pure hydrofluosilicic acid[149] on the fragment

and leave it for some hours in damp air until the action has been

sufficient, then transfer it to a dry air bell-glass and allow

evaporation and crystallization to take place.

For the microscopic examination the objective (200–300 diams. best for

these observations) can be protected with glycerine and a mica disc or

thin cover-glass, or the drop can be all evaporated and the crystals

covered with liquid balsam and a cover-glass.

Crystallizations Obtained by Borichy’s Method.

_Potassium._ From hydrofluosilicic solutions,[150] isotropic, colorless

crystals of K_{2}SiFl_{6}, in cubes, octahedra or combinations of these

forms with the rhombic dodecahedron. Apparently orthorhombic crystals

may form from acid solutions and at a low temperature, but if these

crystals are dissolved in hot water and recrystallized they will assume

the normal forms.

Platinic chloride will produce under proper conditions sharp, yellow

octahedra of K_{2}PtCl_{6}.

[Illustration:

FIG. 78.—Fluosilicate of potassium.[151]

]

[Illustration:

FIG. 79.—Fluosilicate of sodium.[151]

]

_Sodium._ From hydrofluosilicic solutions, colorless, very weakly doubly

refracting, hexagonal crystals of Na_{2}SiFl_{6}, which are generally

longer the higher the percentage of sodium in the solution. This test is

very certain even for small amounts.

[Illustration:

FIG. 80.—Fluosilicate of calcium.[151]

]

[Illustration:

FIG. 81.—Fluosilicate of magnesium.[151]

]

_Calcium._ From hydrofluosilicic solutions, monoclinic crystals of

CaSiFl_{6} + 2H_{2}O of various forms, generally spindle-shaped, with

not very strong double refraction. The crystals have seldom

straight-edged boundaries and are often grouped in rosettes. The

addition of dilute H_{2}SO_{4} decomposes the crystals,

recrystallization yielding long prismatic crystals of gypsum

(distinction from strontium).

Treatment with HFl and dilute H_{2}SO_{4} (in excess), producing on

evaporation characteristic crystals of gypsum, furnishes a very delicate

test for small percentages of calcium.

_Magnesium._ From hydrofluosilicic solutions, rhombohedral crystals of

MgSiFl_{6} + 6H_{2}O with plane faces and sharp edges. The crystals are

colorless and strongly doubly refracting with positive optical

character, Fig. 81.

The formation of struvite crystals (NH_{4}MgPO_{4} + 6H_{2}O), of

coffin-like forms, is very characteristic and takes place from very

dilute solutions (rendered alkaline) on the addition of a grain of salt

of phosphorus or a drop of sodium phosphate.

_Iron._ From hydrofluosilicic solutions, crystals of FeSiFl_{6} +

6H_{2}O, which are isomorphous with those of magnesium salts, with the

same optical characters. They may be differentiated by moistening with

potassium ferrocyanide or ammonium sulphide, in the first case by

turning blue, in the second case black.

_Aluminium._ From hydrofluosilicic solutions, not satisfactory on

account of the gelatinous formation.

When the gelatinous formation is obtained by the action of hydrofluoric

acid on an _aluminous silicate_, the staining test can be used to

distinguish between fine grains of feldspar and quartz or iolite and

quartz.

Behrens’ Method.[152] (Hydrofluoric and Sulphuric Acids.)

This method depends on common reactions that can be made rapidly, but

has the disadvantage of being rather complicated and requiring delicate

manipulation.

The tests are best made upon about ½ mg. of powder with HFl (pure and

fuming). As soon as the fluorides begin to dry treat with dilute

H_{2}SO_{4} and warm until white fumes of SO_{3} appear. In this way the

HFl and SiFl_{4} are driven off and the sulphates are left. This part of

the test can conveniently be made on a piece of platinum foil. Add

excess of water and concentrate.

Transfer a drop to a clean object glass and, while still liquid, examine

it with the microscope. Do not use a cover-glass over the drop.

Crystallizations Obtained by Behrens’ Method.

_Potassium._ Add a little platinic chloride when octahedral crystals of

K_{2}PtCl_{6} (size .18 to .30 mm.) will appear, which are clear, bright

yellow in color with strong refraction.

[Illustration:

FIG. 82.—Potassium platinic chloride.[153]

]

[Illustration:

FIG. 83.—Sulphate of calcium (gypsum).[153]

]

_Sodium._ Use sulphate of cerium and allow a small amount of this

reagent to act through a capillary pipette upon a drop of the solution.

Very small aggregates of brown crystals (size .02 mm.) of the double

sulphate of cerium and sodium are formed, which are clearly visible with

600 diams. If potassium is present the double sulphate of that alkali

will appear in larger, grayish grains (size .05 to .06 mm.). An excess

of H_{2}SO_{4} is to be avoided.

_Calcium._ After a few minutes little gypsum crystals (CaSO_{4} +

2H_{2}O) will appear. In strongly acid solutions the thin acicular

crystals will be grouped in bushes or stars; in neutral solutions the

crystals will have the normal shape of selenite crystals or form

swallow-tailed twins.

_Magnesium._ Use salt of phosphorus dissolved in water and allow it to

mix with the solution (to which has been added ammonium chloride and

ammonia) through a capillary pipette. From a solution containing more

than 5 per cent. of magnesium are first deposited X-shaped skeletons and

rudimentary crystals of Mg.NH_{4}.PO_{4} + 6H_{2}O. If the solution is

more dilute beautiful, sharp, hemimorphic crystals (.10 to .20 mm. in

size) of the orthorhombic system will appear. These crystals often

resemble the roof of a house. The formation of the crystals is assisted

by heat. Iron and manganese phosphates yield crystals of the same type,

but the iron is separated on the addition of ammonia.

_Aluminium._ Use chloride of cæsium. Take a drop of the solution, with

excess of H_{2}SO_{4} driven off, and touch it with a platinum wire that

has been dipped in the melted chloride of cæsium. Large crystals

(.40-.90 mm. in size) of cæsium alum will form, which are octahedral and

cubo-octahedral in shape. Iron does not interfere, as its

crystallization would take place much more slowly. The solution should

not be too concentrated.

[Illustration:

FIG. 84.—Magnesiumammonium phosphate.[154]

]

[Illustration:

FIG. 85.—Cæsium alum.[154]

]

Special Tests.

Distinction between haüynite (contains CaSO_{4}) and noselite (contains

Na_{2}SO_{4}). Treat with HCl and on evaporation the characteristic

crystals of gypsum will be seen if the mineral is haüynite. Dilute acid

should be used and as low a temperature maintained as possible,

otherwise crystals of anhydrite would form instead of gypsum.

Recognition of apatite by test for phosphorus. Treat with a drop of

ammonium molybdate dissolved in HNO_{3}. After complete action remove

the solution to a clean object glass, when after slight warming a large

number of very small yellow crystals (rhombic dodecahedral in shape)

will form. The test may be used to distinguish this mineral from

nephelite, melilite and natrolite. In the presence of soluble silica

evaporate to render it insoluble and treat again with HNO_{3} and the

reagent.

Other micro-chemical tests are not mentioned for the reason that in

elaborate chemical investigations of sections or isolated fragments

recourse should be made to the most complete publications on the

subject.

APPENDIX.

BRIEF SCHEME OF CLASSIFICATION INTO SYSTEMS BY OPTICAL DETERMINATIONS.

▄HOMOGENEOUS.▄ The whole substance shows the same optical

character, except in the case of twin crystals when

the different portions of the twin are affected

differently.

▄Isotropic▄ All sections of the substance remain dark during a

complete rotation between crossed nicols, and no

interference figure is produced by convergent light.

Amorphous Absence of crystalline form or cleavage.

Isometric Presence of crystalline form or cleavage.

▄Anisotropic.▄ Sections generally show some interference color and

extinguish four times, at 90° apart, during complete

rotation.

_Uniaxial._ Determined by character of interference figures

obtained by convergent light from sections which

remain dark or nearly so during complete rotation.

All sections show parallel or symmetrical

extinction.

Tetragonal Sections giving interference figures are four- or

eight-sided, or show rectangular cleavage.

Hexagonal Sections giving interference figures are three-,

six- or nine-sided, or show cleavage lines

intersecting at 60°.

_Biaxial_ Determined by character of interference figures

obtained by convergent light.

Orthorhombic Extinction is parallel or symmetrical in all

sections parallel to _ă_, [_=b_] and _ć_. Color

distribution is symmetrical to two lines and to the

central point, see p. 48.

Monoclinic Extinction is only parallel or symmetrical in

sections parallel to the ortho axis [_=b_]; all

other sections show extinction angles. Color

distribution is only symmetrical to one line or to

the central point, see p. 48.

Triclinic Extinction angles in all sections, although in some

minerals these angles may be very small. No symmetry

in color distribution, see p. 48.

▄AGGREGATE.▄ Not homogeneous, but made up of an aggregation of

individuals, all extinguishing at different times.

Double Refraction (maximum).[155]

0.287 Rutile

0.179 Dolomite

0.172 Calcite

0.141 Titanite

0.090 Titanite

0.072 Hornblende (basaltic)

0.062 Zircon

0.058 Biotite

0.050 Talc

0.050 Ægirite

0.041 Muscovite

0.037 Epidote

0.036 Chrysolite (Olivine)

0.036 Scapolite (Meionite)

0.034 Tourmaline

0.034 Phlogopite

0.030 Allanite (Orthite)

0.029 Diopside

0.027 Actinolite

0.027 Tremolite

0.024 Hornblende (common)

0.024 Diallage

0.024 Anthophyllite

0.023 Augite

0.021 Sillimanite (Fibrolite)

0.018 Glaucophane

0.017 Tourmaline (precious)

0.016 Cyanite (Disthene)

0.013 Hypersthene

0.013 Scapolite (Marialite)

0.013 Anorthite

0.012 Natrolite

0.011 Chlorite (Clinochlore)

0.011 Andalusite

0.011 Topaz

0.010 Staurolite

0.010 Gypsum

0.010 Enstatite

0.010 Serpentine

0.009 Corundum

0.009 Iolite (Cordierite)

0.009 Quartz

0.008 Topaz

0.008 Kaolin

0.008 Labradorite, Ab_{1}An_{1}

0.008 Oligoclase, Ab_{4}An_{1}

0.008 Albite

0.007 Orthoclase

0.007 Microcline

0.006 Vesuvianite

0.005 Zoisite

0.004 Nephelite (Elæolite)

0.003 Apatite

0.003 Melilite

0.002 Tridymite

0.002 Leucite

0.002 Allanite (Orthite)

0.001 Chlorite (Penninite)

0.001 Vesuvianite

Indices of Refraction (mean).[155]

2.712 Rutile

2.38 Perofskite

2.00 Spinel (Chrome)

1.963 Titanite

1.95 Zircon

1.920 Titanite

1.856 Garnet (Melanite)

1.792 Ægirite

1.78 Allanite (Orthite)

1.78 Garnet (Almandite)

1.766 Corundum

1.751 Epidote

1.75 Garnet (Pyrope)

1.741 Staurolite

1.723 Hypersthene

1.72 Spinel

1.720 Zoisite

1.720 Cyanite (Disthene)

1.719 Hornblende (basaltic)

1.715 Vesuvianite

1.711 Augite

1.699 Zoisite

1.697 Diopside

1.688 Diallage

1.675 Chrysolite (Olivine)

1.665 Enstatite

1.664 Sillimanite (Fibrolite)

1.674 Tourmaline

1.644 Anthophyllite

1.64 Hornblende (common)

1.637 Andalusite

1.635 Apatite

1.632 Glaucophane

1.632 Topaz

1.630 Melilite

1.633 Tourmaline (precious)

1.622 Dolomite

1.621 Actinolite

1.621 Tremolite

1.618 Biotite

1.608 Topaz

1.588 Chlorite (Clinochlore)

1.587 Muscovite

1.582 Anorthite

1.576 Chlorite (Penninite)

1.572 Talc

1.584 Scapolite (Meionite)

1.564 Phlogopite

1.56 Serpentine

1.559 Labradorite, Ab_{1}An_{1}

1.55 Kaolin

1.547 Quartz

1.551 Scapolite (Marialite)

1.601 Calcite

1.541 Oligoclase, Ab_{4}An_{1}

▄1.54▄ + ▄Canada balsam▄

1.539 Nephelite (Elæolite)

1.539 Iolite (Cordierite)

1.535 Albite

1.525 Gypsum

1.525 Microcline

1.523 Orthoclase

1.509 Leucite

1.503 Haüynite

1.488 Analcite

1.483 Natrolite

1.483 Sodalite

1.477 Tridymite

1.46 Opal

[Illustration:

Diagram showing relation between strength of Double Refraction,

Interference Colors and Thickness of Section.[156]

]

ORDER OF CONSOLIDATION OF THE CONSTITUENT MINERALS IN PLUTONIC ROCKS.

“There is in plutonic rocks a normal order of consolidation for the

several constituents, which holds good with a high degree of generality.

It is in the main, as pointed out by Rosenbusch, a law of ‘decreasing

basicity.’ The order is briefly as follows:

“1. Minor accessories (apatite, zircon, sphene, garnet, etc.) and iron

ores.

“2. Ferro-magnesian minerals—olivine, rhombic pyroxenes, augite,

ægirine, hornblende, biotite, muscovite.

“3. Felspathic minerals—plagioclase felspars (in order from anorthite to

albite), orthoclase (and anorthoclase).

“4. Quartz, and finally microcline.

“In most rocks such minerals as are present follow the above order. The

most important exceptions are the intergrowth of orthoclase and quartz

and the crystallization of quartz in advance of orthoclase in some acid

rocks, and the rather variable relations between groups 2 and 3 in some

more basic rocks. The order laid down applies in general to parallel

intergrowths of allied minerals; thus when augite is intergrown with

ægirine or hornblende the former mineral forms the kernel of the complex

crystal and the latter the outer shell; when a plagioclase crystal

consists of successive layers of different compositions the layers

become progressively more acid from the center to the margin.

“Certain constituents having variable relations are omitted from the

foregoing list. Thus nepheline (elæolite) and sodalite belong to group

3, but may crystallize out either before or after the feldspar.”[157]

OPTICAL SCHEME.

INTRODUCTION.

The scheme is designed to furnish the student with a practical method of

recognizing the common minerals in rock sections.

The arrangement followed has been to group minerals having general

optical characters in common, at the same time giving their specific

characters so as to make it possible to distinguish one from another. In

each rectangle the minerals are arranged in order of their indices of

refraction.

A tabulation of the minerals, with a list of optical characters

appended, is of aid to the skilled investigator, but of very little

assistance to the beginner.

The more common minerals, or those which are important petrographically,

are printed in heavy-faced type; the minerals of less importance in

small capitals.

ABBREVIATIONS AND CONVENTIONS USED.

A. = Amorphous.

I. = Isometric system.

T. = Tetragonal system.

O. = Orthorhombic system.

M. = Monoclinic system.

Tri. = Triclinic system.

H. = Hexagonal system.

M(H). = Monoclinic, with hexagonal form or characters, as in the case

of biotite.

⟂ = At right angles to.

El. = Elongation.

Ex. = Extinction.

∥ Ex. = Parallel extinction, as when the crystals extinguish parallel

to cleavage lines or crystal edges. Extinction which is symmetrical to

intersecting cleavage lines is also included under this term.

The mean refractive indices are printed in heavy-faced type.

The term “grains” is used to describe not only minerals which occur in

typically granular form, but also those which have coarser

allotriomorphic form, as elæolite and sodalite in plutonic rocks, such

as syenite, etc.

GENERAL RULES FOR USE OF SCHEME.

The division of the scheme into two vertical columns is based on the

values of the mean refractive indices, as determined by the “relief” and

appearance of the surface. When the refractive index is above 1.60, the

relief is fairly well to distinctly marked and the surface rough to very

rough, depending on the value of the index.

Most of the rock-forming minerals with indices below 1.60 show no relief

and a smooth surface, except in the case of a few of the rarer minerals

(mostly isometric), which have very low indices and hence rough surface.

Mistakes may easily be made in the case of minerals near the limit; but

practice and the use of the Becke test should soon make possible the

classification into the two groups suggested by the scheme, and the

appended descriptions will help to check errors.

When an unknown mineral lies adjacent to one that is known, use the

Becke test for obtaining the relative refractive index of the unknown

mineral; focus sharply on the line of contact between the known and

unknown minerals,[158] then raise the objective slightly and the “bright

line” will appear on the side of the mineral having the higher index.

The method of Schrœder van der Kolk may also be employed, see p. 22.

The horizontal divisions of the scheme depend on the relative strength

of the double refraction based on the observed interference colors.

These colors to be of use in classification must be correctly

recognized. The lower and middle colors of the 1° order, from

bluish-gray through white to yellow, are easily known. The bright red,

blue, green, etc., colors of the 1°, 2° and 3° orders can also be

differentiated without trouble from the very high order colors (4° and

above), which are essentially white in tone with no decided color tint.

When confusion arises, the exact order of the color can be determined by

a quartz wedge, as given on p. 35. Furthermore, a ¼ undulation mica

plate serves to quickly distinguish between the 1° order white and the

practically colorless, high order tint of calcite, titanite, etc.; as

after the insertion of the test-plate the 1° order white suffers a

marked change in color, while the very high order (practically white)

tint shows no appreciable change.

In the determination of these interference colors care must be given to

considerations of orientation and thickness. The section must give the

maximum interference color of all the obtainable sections of the mineral

in the rock section. Such sections will be parallel to the _ć_ axis in

the uniaxial minerals and to the axial plane in the biaxial minerals;

and will, therefore, in convergent light never show the emergence of an

optic axis or bisectrix. Crystal “form,” cleavage, pleochroism, etc.,

may at times aid in the selection of these sections. The thickness of

the section must also be considered, and it is well in all cases to pick

out some known mineral in the section, as quartz, and note its maximum

interference color. Knowing how this varies from the color given by the

scheme for a section 0.03 mm.[159] in thickness, due allowance can be

made for a like variation in the colors given by the other minerals. In

the case of minerals with strong absorption the interference colors may

not be noticeable on account of the absorption of parts of the light.

Under the subhead of pleochroism, the vibration direction of the ray of

a definite color is given and not the direction of transmission of that

ray.

The interference figures in convergent light increase in clearness and

distinctness with the strength of the double refraction. In uniaxial

crystals sections at right angles to the optic axis, _i. e._, sections

which remain dark during a revolution between crossed nicols, show the

best interference figures. In biaxial crystals the most characteristic

interference figures are shown by sections at right angles to the acute

bisectrix.

Crystal sections which are too small do not give very satisfactory

interference figures with convergent light.[160]

Any scheme, however designed, makes a more or less arbitrary

classification of the minerals, and when in doubt it is always safer to

look for the mineral on both sides of the scheme line.

The rarer minerals are not included in this scheme, so when the

determination of a mineral is uncertain or not positive recourse should

be had to more elaborate tables.

INDEX.

MINERAL NAMES IN HEAVY-FACED TYPE.

Abbreviations, ix

Abnormal interference colors, 30

Absorption, 26

directions, 26

tints, 17

▄Acmite▄, 83

▄Actinolite▄, 84

Acute bisectrix, 5

▄Ægirine▄, 83

▄Ægirine-augite▄, 84

Aggregate structure, 38

▄Albite▄, 103

▄Allanite▄, 96

Allotriomorphic, 15

Aluminium, test for, by Borichy’s method, 137

test for, by Behren’s method, 139

Amorphous bodies, 2

Amorphous substances, test for, 26

▄Amphibole▄, 84

▄Analcite▄, 56

Analyzer, 10

▄Andalusite▄, 72

Anhedron, 15

Anisotropic character, test for, 27

Anisotropic crystals, 2

Anomalies, optical, 27

▄Anorthite▄, 103

▄Anorthoclase▄, 113

▄Anthophyllite▄, 88

▄Antigorite▄, 114

▄Apatite▄, 68

Apatite, recognition of, by test for phosphorus, 139

Apparatus for petrographical laboratory, 127

Appendix, 141

▄Arfvedsonite▄, 88

▄Augite▄, 80

Automorphic, 13

Axes of elasticity, 4

Axial angle, 5

determination of, 47

Axial plane, 5

▄Basaltic Hornblende▄, 85

▄Bastite▄, 77

Becke’s method for determining relative values of refractive indices,

19

Behren’s method. (Hydrofluoric and sulphuric acids), 137

Bertrand lens, 11

Biaxial crystals, 4, 5

vibration directions in, 4

Biaxial interference figures, 43

▄Biotite▄, 89

Bisectrix, acute, 5

obtuse, 5

Borichy’s method. (Hydrofluosilicic acid), 135

Broken or strained crystals, 15

▄Bronzite▄, 76

▄Calcite▄, 65

Calcium, test for, by Borichy’s method, 136

test for, by Behren’s method, 138

“Cap” nicol, 10

▄Carbonaceous Matter▄, 61

Carbonaceous particles, test for, 132

Carbonates, test for, 130

Cement, 122

for mounting, 126

Cementing, 121

Centering stage, 10

▄Chalcedony▄, 64

Characters observed by, convergent light, 40

crossed nicols, 26

reflected light, 13

polarized light, 25

Characters of opaque minerals, 13

transparent minerals, 13

Chemical and mechanical tests, 129

Chemical (micro) reactions, 134

separation, 134

tests on crystal in section, 129

▄Chiastolite▄, 72

▄Chlorite group▄, 92

▄Chromite▄, 52

▄Chrysolite▄, 77

▄Chrysotile▄, 114

Circular polarization, 3

Classification into systems by optical determinations, 141

▄Clay▄, 115

Cleaning and finishing sections, 126

Cleaning microscope, 11

Cleavage, 23

▄Clinozoisite▄, 96

Color, 17

diagram (interference), 143

fringes, 48

Condensing lens, 9

Consolidation of minerals in plutonic rocks, order of, 144

Conventions, ix

Convergent light, 40

characters observed by, 40

Convergent and parallel light, résumé of uses of, 49

▄Cordierite▄, 78

Corroded crystals, 15

▄Corundum▄, 62

Crossed nicols, characters observed by, 26

Crossed twinning, 37

Crystallites, 16

Crystallizations obtained by Behren’s method, 137

Borichy’s method, 135

Crystals bounded by planes, 13

Crystals without bounding planes, 15

Cutting, 120

Cutting and grinding machines, 117

▄Cyanite▄, 113

▄Damourite▄, 92

▄Delessite▄, 94

Diagram, showing relation between strength of double refraction,

interference colors and thickness of section, 143

▄Diallage▄, 80

Diamond saws, 119

▄Dichroite▄, 78

▄Diopside▄, 80

▄Dipyre▄, 59

Directions of elasticity, ix

Dispersion, 5, 48

▄Disthene▄, 113

▄Dolomite▄, 67

Double image, 2

Double refraction, 2, 27

estimation of strength of, 30

strength of, measured by von Federow mica wedge, 35

table (maximum), 142

Effects produced by crystals on transmitted light, 2

▄Elæolite▄, 69

Elasticity, axes of, 4

directions of, ix

Electric motor for grinding machines, 117

Electro-magnetic separation, 134

Emery, grades of, for grinding, 124

▄Enstatite▄, 75

▄Epidote▄, 94

Etched figures, 130

Extinction, 31

angles, 5, 31

tests for, 32

wavy, 31

Extraordinary ray, 3

Eye-pieces, 11

Faster and slower rays, test for vibration directions of, 33

▄Fayalite▄, 78

▄Feldspar Group▄, 98

Feldspathoids, 69

▄Fibrolite▄, 73

Finishing and cleaning sections, 126

Focusing, 11

Form of crystals, 13

Fracture, 24

▄Garnet▄, 53

Gelatinizing silica, test for, 130

Glass slides, 125

▄Glaucophane▄, 88

▄Graphite▄, 61

Gravity (specific) separation, 133

Gridiron twinning, 37

Grinding, 123

Grinding and cutting machines, 117

apparatus for sections with parallel faces, 118

plates or laps, 121

▄Gypsum▄, 80

Gypsum test-plate, 33

Hardness of grains, 132

▄Haüyne▄, 56

▄Haüynite▄, 56

Haüynite and noselite, micro-chemical distinction between, 139

Heating sections to redness, 131

Heavy solutions, 133

▄Hematite▄, 61

Hexagonal crystals, 4

High relief, 17

▄Hornblende▄, 84

▄Hyalosiderite▄, 78

▄Hydrargillite▄, 115

Hydrofluosilicic acid test, 135

▄Hypersthene▄, 75

Idiomorphic, 13

▄Idocrase▄, 60

▄Ilmenite▄, 62

Inclusions, 24

Index of refraction, ix, 17

by Becke’s method, 19

by Schrœder van der Kolk’s method, 22

by Sorby’s method, 19

Indicators for specific gravity separation, 133

Indices of refraction (mean), table of, 142

Interference color, determination of order of, 35

Interference colors, 28

Interference colors (abnormal), 30

Interference figures, 40

biaxial, 43

uniaxial, 40

Investigation of microscopic and optical characters of minerals, 13

▄Iolite▄, 78

Iron, test for, by Borichy’s method, 137

test for, by Behren’s method, 139

Isolating crystals or mineral fragments for testing, 132

Isometric crystals, 2

Isotropic character, 26, 40

crystals, 2

▄Kaolin▄, 115

▄Labradorite▄, 103

Laps for grinding, 121

▄Leucite▄, 54

Leucoxene, 62

Light, ordinary, 1

plane polarized, 1

▄Limonite▄, 51

▄Lithia Mica▄, 92

Machines for cutting and grinding, 117

Magnesium, test for, by Borichy’s method, 137

test for, by Behren’s method, 138

▄Magnetic iron ore▄, 52

▄Magnetic pyrites▄, 51

▄Magnetite▄, 52

Measuring strength of double refraction by von Federow mica wedge, 35

Mechanical and chemical tests, 129

▄Melilite▄, 61

▄Menaccanite▄, 62

Methods of preparing sections, 117

▄Mica Group▄, 89

Mica plate (quarter undulation), 33

Mica wedge, von Federow, 35

Micro-chemical reactions, 134

▄Microcline▄, 102

Microlites, 17

Microscope (petrographical), 7

Microscopic and optical characters of minerals, 51

Minerals and thickness of section, determined by table and diagram, 36

Monoclinic crystals, 4

principal vibration directions in, 5

▄Monoclinic pyroxenes▄, 80

Mounting sections, 124

solutions, 125

▄Muscovite▄, 89

▄Natrolite▄, 79

Negative optical character, biaxial, 46

uniaxial, 42

▄Nepheline▄, 69

▄Nephelite▄, 69

Nicol prism, 7

▄Nosean▄, 56

▄Noselite▄, 56

Noselite and haüynite, micro-chemical distinction between, 139

Nose-piece for microscope, 10

Objectives, 10

Oblique extinction, 31

Obtuse bisectrix, 5

▄Oligoclase▄, 103

▄Olivine▄, 77

▄Opal▄, 51

Opaque minerals, characters of, 13

Optical, anomalies, 27

character, biaxial, 46

character, uniaxial, 42

classification into systems, 141

distinctions between orthorhombic, monoclinic and triclinic sections

(perpendicular to bisectrices), 48, 141

distinctions between tetragonal and hexagonal sections (perpendicular

to optic axis), 141

and microscopic characters of minerals, 51

principal section, 3, 4

scheme, 145

Optic axes, 4

Optic axis, 3

Optics for optical mineralogy, 1

Order of consolidation of minerals in plutonic rocks, 144

Order of interference color, determination of, 35

Ordinary light, 1

ray, 3

▄Orthite▄, 96

▄Orthoclase▄, 98

Orthorhombic crystals, 4

principal vibration directions in, 4

▄Orthorhombic pyroxenes▄, 75

Parallel and convergent light, résumé of uses of, 49

Parallel extinction, 31

Parallel face sections, grinding apparatus for, 119

▄Pargasite▄, 85

▄Perofskite▄, 57

▄Perovskite▄, 57

Petrographical apparatus, 127

Petrographical microscope, 7

Phenocryst, 14

▄Phlogopite▄, 89

▄Picotite▄, 53

▄Piedmontite▄, 95

▄Plagioclases▄, 103

Plane polarized light, 1

Plates, grinding, 121

Pleochroic halos, 59

Pleochroism, 25

test for, 25

▄Pleonaste▄, 53

Polarization colors, 28

Polarized light, characters observed by, 25

plane, 1

Polarizer, 7

test for vibration plane of, 9

Polishing sections, 124

Polysynthetic twinning, 37

Positive optical character, biaxial, 46

uniaxial, 42

Potassium, test for, by Borichy’s method, 136

test for, by Behren’s method, 138

Preparation of sections, 117

Principal section, optical, 3, 4

Principal vibration directions, 3, 4

Prism, nicol, 7

Pseudomorphic structure, 39

▄Pyrite▄, 51

▄Pyrites▄, 51

▄Pyroxenes, monoclinic▄, 80

▄Pyroxenes, orthorhombic▄, 75

▄Pyrrhotite▄, 51

Quarter-undulation mica plate, 33

▄Quartz▄, 63

wedge, 34

Reflected light, characters observed by, 13

Reflector, 7

Refraction, double, 2, 27

Refraction, index of, ix, 17

Refractive indices (mean), table of, 142

Relief, 17

test for, 17, 18

Resorption border, 15

Résumé of uses of parallel and convergent light, 49

Rotating stage of microscope, 10

▄Rutile▄, 57

▄Sagenite▄, 58

▄Sanidine▄, 102

▄Saussurite▄, 96, 113

Saws, 119

▄Scapolite Group▄, 59

Scheme of classification into systems by optical determinations, 141

Scheme, optical, 145

Schiller structure, 25

Schrœder van der Kolk’s method for determining refractive indices, 22

Sections, methods of preparing, 117

thickness of rock, 124

Selenite plate, 33

Separation, by chemical means, 134

by electro-magnet, 134

by specific gravity, 133

▄Sericite▄, 92

▄Serpentine▄, 114

Shagreened surface, 17

▄Shorl▄, 70

▄Sillimanite▄, 73

Simple twinning, 37

Single image, 2

Skeleton forms, 17

Slides, glass, 125

Slower and faster rays, test for vibration directions of, 33

▄Sodalite▄, 56

▄Sodalite Group▄, 56

Sodium, test for, by Borichy’s method, 136

test for, by Behren’s method, 138

Sorby’s method for determining index of refraction, 19

Special micro-chemical tests, 139

Specific gravity separation, indicators for, 133

Sphærulitic structure, 39

▄Sphene▄, 96

▄Spinel▄, 53

Stage of microscope, rotating, 10

▄Staurolite▄, 74

Strained or broken crystals, 15

Strength of double refraction, measure of, 30, 35

Structure, 37

Symmetrical extinction, 31

Systems, classification into, by optical determinations, 141

Table, double refraction, 142

Table, indices of refraction, 142

▄Talc▄, 94

Test for vibration plane of polarizer, 9

Tetragonal crystals, 4

Thickness of rock sections, 124

Thickness of section and minerals, determined by table and diagram, 36

▄Titanite▄, 96

Transmitted light, characters observed by, 13

effect on crystals, 2

Transparent minerals, investigation of characters of, 13

▄Tremolite▄, 84

Triclinic crystals, 4

principal vibration directions in, 5

▄Tridymite▄, 65

▄Topaz▄, 74

▄Tourmaline▄, 70

Twinning, 37

Uniaxial crystals, vibration directions in, 3

Uniaxial interference figures, 40

▄Uralite▄, 88

Uralitization, 88

Uses of parallel and convergent light, 49

van der Kolk’s, Schrœder, method for determining refractive indices, 22

▄Vesuvianite▄, 60

Vibration direction, 2

directions of faster and slower rays, test for, 33

directions, principal, 3, 4

plane of nicol, 9

plane of polarizer, test for, 9

von Federow mica wedge, 35

Wavy extinction, 16, 31

Wedge, mica, 35

quartz, 34

▄Wernerite▄, 59

Xenomorphic, 15

▄Zeolites▄, 79

▄Zircon▄, 58

▄Zoisite▄, 96

α and β, 96

Zonal structure, 38

ERRATA AND ADDENDA.

P. 33, line 23, _for_ beat _read_ be at.

P. 66, line 10, _after_ appearance _add_ (sometimes called “twinkling”).

Corrections for mean index of refraction _n′_: p. 60, line 1, 1.551 to

1.584; p. 62, line 29, 1.766; p. 66, line 3, 1.601; p. 67, line 24,

1.622; p. 71, line 10, 1.633 to 1.674.

Corrections for Indices of Refraction (mean) in Table on p. 142:

Corundum 1.766; Tourmaline 1.674; Tourmaline (precious) 1.633; Dolomite

1.622; Scapolite (Meionite) 1.584; Scapolite (Marialite) 1.551; Calcite

1.601.

Corrections for mean indices of refraction in Scheme (insert folder):

Scapolite 1.551 to 1.584; Calcite 1.601 and transfer to Dolomite

rectangle; Dolomite 1.622; Corundum 1.766; Tourmaline 1.633 to 1.674.

-----

Footnote 1:

Often called a direction of maximum elasticity, c′ being a direction

of minimum elasticity.

Footnote 2:

Rosenbusch’s _Microskopische Physiographie_, p. 156.

Footnote 3:

For a more complete discussion of optics, in connection with Optical

Mineralogy, the student is referred to A. J. Moses’ _Characters of

Crystals_, p. 85, et seq.; Moses’ & Parsons’ _Mineralogy,

Crystallography and Blowpipe Analysis_, Chap. XVI., 4th Ed., 1909;

Miers’ _Mineralogy_, 1902; L. Fletcher’s _Optical Indicatrix_, etc.,

1892; Groth’s _Physikalische Krystallographie_, 3d Ed.; Rosenbusch’s

_Mikroskopische Physiographie_, 4th Ed. and Iddings’ _Rock Minerals_,

1911.

Footnote 4:

The electromagnetic theory of light is now very generally held, but,

whatever may be the recurrent change of state to which light is really

due, the principles of wave motion furnish a satisfactory geometric

description of optical phenomena.

Footnote 5:

These sections are supposed to have plane parallel faces, such being

the case in ordinary practice, and to be examined with parallel

perpendicularly incident light.

Footnote 6:

It is interesting to remember in this connection that in the isometric

system there is also the greatest possible symmetry of “form.”

Footnote 7:

A. J. Moses, _Characters of Crystals_, pp. 85–97.

Footnote 8:

For this branch of optical physics, see A. J. Moses, _Characters of

Crystals_, pp. 97–100.

Footnote 9:

This can be demonstrated by using a nicol and a plate of calcite which

shows a double image. If the nicol is held between the calcite plate

and the observer’s eye it can be so adjusted that only one image is

seen. If now the nicol is revolved 90° the first image will disappear

and the other image alone will be seen.

Footnote 10:

In some cases a peculiar form of double refraction does take place

parallel to this direction, as in the circular polarization of quartz

and cinnabar; but in very thin sections these results are not noticed

and can be disregarded.

Footnote 11:

A. J. Moses, _Characters of Crystals_, pp. 98, 99.

Footnote 12:

The terms axes of elasticity are commonly used for these principal

vibration directions in text-books on petrography.

Footnote 13:

Instead of ω and ε, for convenience in tables, etc., α and γ are used,

denoting the indices of refraction of the rays traversing the crystal

with greatest and least velocity respectively, without regard as to

which is the _O_ or _E_ ray. A good reason for this convention is that

the symbol (γ − α) is used to express in decimals the relative

strength of the double refraction of a crystal, whether uniaxial or

biaxial. γ is always greater than α.

Footnote 14:

For most cases in observations with white light the “optics axes” may

be regarded as approximately fixed in position.

Footnote 15:

Often spoken of as: a, the axis of maximum; b, the axis of

intermediate, and c, the axis of minimum elasticity.

In the more recent American text-books on Optical Mineralogy by

Iddings, Winchell and Phillips a is denoted by _X_, b by _Y_ and c by

_Z_.

Footnote 16:

For a short historical sketch of the use of the microscope in

connection with Petrology, see G. H. William’s pamphlet, _Modern

Petrography (Monographs of Education)_, Boston, 1886. For detail

description and adjustments, see _Methods of Petrographic-Microscopic

Research_, F. E. Wright, 1911, pp. 11, 61.

Footnote 17:

For description of the ordinary microscope, eye-pieces, objectives,

magnification, etc., see _Manipulation of the Microscope_, by Ed.

Bausch.

Footnote 18:

Text Book of Mineralogy, by E. S. Dana, 1898 Ed., p. 176.

Footnote 19:

It is convenient to assume that the vibrations of the polarized light

are taking place in this plane, called the “plane of vibration,” but

all the phenomena caused by polarized light could be also explained on

the assumption that the vibrations were taking place at right angles

to this plane.

Footnote 20:

This condensing lens must be removed when very low power objectives

are used.

Footnote 21:

Some microscopes are provided with adjusting screws bearing on the

frame holding the objective, which can then be accurately centered to

the axis of rotation of the stage.

Footnote 22:

In the Seibert microscope use objective No. 00 for the first general

study of a rock section, No. II for general use and No. V for

observations with convergent light. In the Fuess microscope use

objective No. 4 for general use and No. 7 for convergent light tests.

In the case of an English microscope a 1″ to ¾″ objective is used for

general purposes and a ¼″ to ⅕″ for observations with convergent

light.

Footnote 23:

See pp. 33 and 34.

Footnote 24:

In some microscopes the analyzer is in the form of a “cap” nicol,

arranged to be fitted over the top of the eye-piece, and not

introduced in the microscope tube as shown here. This form is not so

convenient, as the “cap” nicol must be set by hand every time it is

desired to make observations with crossed nicols. But at the same time

it avoids any possible refocusing which may be necessary when the

other type of analyzer is introduced in the tube.

Footnote 25:

When accurate adjustments are possible of the vibration planes of the

nicols and the cross-wires parallel to these vibration planes,

reference should be made to _Methods of Petrographic-Microscopic

Research_, p. 61, 1911, Fred. E. Wright.

Footnote 26:

In the Seibert microscope eye-piece No. 0 is used for most purposes.

Other eye-pieces, Nos. 1 and 2, with cross-wires, are used for

different degrees of magnification, and one eye-piece, No. 3, without

cross-wires, is provided to be used in connection with an eye-piece

micrometer.

Footnote 27:

With the Seibert microscope, Fig. 2, the No. 0 eye-piece and the No.

II objective will prove most satisfactory for the following tests.

With the Fuess microscope use No. 4 objective. With an English

microscope use an ordinary eye-piece and a 1″ or ¾″ objective.

Footnote 28:

Twins may be recognized just as in macroscopic specimens, and zonal

structure noticed if the zones differ in color. When a colorless

mineral is surrounded by other colorless minerals, of about the same

index of refraction, its outline is often best brought out by

observation between crossed nicols.

Footnote 29:

The term “Anhedron,” meaning without planes, has been suggested by L.

V. Pirsson to describe in rocks the crystal fragments which have no

plane faces, as, for example, the augites of augitic rocks. _Science_,

Jan. 10, 1896, p. 49.

Footnote 30:

Partial resorption and recrystallization may produce a border of

secondary minerals, surrounding the original crystal.

Footnote 31:

The surfaces of all minerals in sections are more or less rough, but

this roughness is only made visible when there is a marked difference

between the indices of refraction of the minerals, and the index of

refraction of the balsam in which the minerals are embedded. The index

of refraction of balsam is about 1.54, so it is only when the mineral

has a higher or lower index of refraction that its surface appears

rough. When internal structure is to be studied, the crystal should be

surrounded by a fluid of nearly the same index of refraction as that

of the crystal, and when the exterior of the crystal is to be studied,

then a fluid should be used with a very different index of refraction.

Footnote 32:

The Seibert microscope has a very convenient and quick lowering

adjustment, by means of the lever _d_, for making this test. For

convenience the lower nicol and condensing lens are generally left in

place below the stage of the microscope, as polarized light serves as

well for these investigations as ordinary light. An additional

advantage in this arrangement is that the condensing lens is always

ready for the “relief” test and the lower nicol for the pleochroism

test; but it must be remembered that the polarizer or lower nicol cuts

out one half of the light, which comes to it from the reflector, and

this loss is important when high power objectives are to be used. When

very low power objectives are used, the condensing lens must be

removed.

Footnote 33:

_Mem. de l’Acad._, Paris, 1767–68.

Footnote 34:

_Min. Mag._, Vol. I., p. 193; Vol. II., p. 1.

Footnote 35:

_Sitzungsberichte der k. k. Akad. der Wiss._, Wien, 1893, I Abt., p.

358. Translation by L. McI. Luquer in _School of Mines Quarterly_,

Vol. XXIII., Jan., 1902, No. 2, p. 127. Review by Viola in _Min. Pet.

Mitt._, Vol. 14, p. 554. _Methods of Petrographic-Microscopic

Research_, F. E. Wright, 1911, p. 95.

Footnote 36:

Most of the petrographical microscopes carry over the polarizer a

convex lens the effect of which is to widen the illuminating cone and

hence make less visible this phenomenon.

Footnote 37:

In Seibert student microscope, No. II _a_, use next to smallest

light-stop. Some of the Fuess microscopes are supplied with an

iris-blende for limiting the cone of light.

Footnote 38:

In Seibert microscope use No. V, not sufficiently marked results being

obtained with No. II.

Footnote 39:

See Viola’s diagram, _Minn. Pet. Mitt._, Vol. XIV., p. 556.

Footnote 40:

Seibert, No. II. Fuess, No. 4.

Footnote 41:

_Kurze Anleitung zur mikrosk._ _Krystallbestimmung_, Wiesbaden, 1898,

and _Tabellen zur mikrosk._ _Bestimmung_, etc., Wiesbaden, 1900.

_Methods of Petrographic-Microscopic Research,_ F. E. Wright, 1911, p.

93.

This method is particularly favorable for the accurate determination

of the refractive indices of small isolated fragments or grains, by

using liquids of known indices. In this case a bright line appears on

the “near” edge and a dark line on the “far” edge if the grain has a

higher index than the liquid. The reverse occurs when the index is

lower than the liquid. When the index is the same (using white light)

the “far” edge is blue and the “near” edge red and also the contours

about disappear.

F. Krantz, of Bonn, furnishes a series of 21 liquids in small bottles,

with indices from 1.447 to 1.83.

The indices of a few convenient liquids are: water, 1.34; alcohol,

1.36; glycerine, 1.41; olive oil, 1.47; nut oil, 1.50; clove oil,

1.54; aniseed oil, 1.58; almond oil, 1.60; cassia oil, 1.63;

monobromnapthalene, 1.65; methylene iodide, 1.75.

Footnote 42:

Crystals that have two good cleavages often develop so that the

direction of elongation is parallel to the intersection of the two

cleavages, while in the case of crystals with one good cleavage the

tendency seems to be towards a tabular habit parallel to the cleavage.

Footnote 43:

Harker’s _Petrology for Students_, p. 306.

Footnote 44:

The lower nicol is generally so adjusted that its plane of vibration

is parallel to the north and south cross-wire in the eye-piece. This

adjustment can be tested by means of a section of biotite, showing

cleavage cracks. When the plane of vibration of the polarizer is

parallel to the N. and S. cross-wire in the eye-piece, the biotite

section becomes almost dark when its cleavage cracks are parallel to

the same cross-wire. The upper nicol, or analyzer, must, of course, be

removed during this test. This method is more convenient than taking

the nicol out of its frame, in order to ascertain its plane of

vibration (the direction of its shorter diagonal).

Footnote 45:

Although the “absorption directions” may not necessarily coincide with

the principal vibration directions in Monoclinic and Triclinic

crystals; still for convenience the absorption colors are usually

given for the light rays vibrating parallel to these principal

vibration directions.

Footnote 46:

In the Fuess and Seibert microscopes the analyzer or upper nicol is so

fitted that it slides in and out of the tube of the microscope with

its plane of vibration always at right angles to the plane of

vibration of the polarizer or lower nicol.

Footnote 47:

Moses’ _Characters of Crystals_, p. 106. Moses and Parsons’ _Min.

Cryst._ and _B. P. Analysis_, p. 163.

Footnote 48:

Iddings’ _Rock Minerals_, 1911, p. 172.

Footnote 49:

These sections always contain the principal vibration directions _a_

and _c_.

Footnote 50:

_Methods of Petrographic-Microscopic Research_, F. E. Wright, 1911, p.

101.

Footnote 51:

A chart of interference colors can be obtained from Baudry et Cie,

Paris, and is also published in _Les Minéraux des Roches_, by Lévy and

Lacroix, _Rock Minerals_ (1911), by Iddings and in Rosenbusch’s

_Mikroskopische Physiographie_.

Footnote 52:

Iddings’ _Rock Minerals_, 1911, pp. 141, 183.

Footnote 53:

_Methods of Petrographic-Microscopic Research_, F. E. Wright, 1911, p.

132.

Footnote 54:

The ¼ undulation mica plate consists of a thin cleavage of mica on

which is marked _c_, the vibration direction of the slower ray, which

in mica is the line joining the “optic axes.” The thickness is such

that the slower ray is ¼ wave-length behind the faster and the

interference color is a bluish-gray. The gypsum plate is a thin

cleavage of gypsum, on which is usually marked a, the vibration

direction of the faster ray. The chosen thickness is such as to

produce the red interference color of the 1° order.

Footnote 55:

The test-plates are generally introduced in the slot _k_, in a

microscope of the Seibert type, or if a cap-nicol is used in a slot

below this. In case no provision is made by the instrument maker for

these test-plates, the regular analyzer is left out of the tube, and a

simple nicol prism is used as an analyzer and is held by the observer

over the eye-piece. Care must be taken to have the plane of vibration

of this nicol at right angles to that of the polarizer, and to leave

sufficient room for the introduction, by hand, of the test-plate

between the eye-piece and the nicol. With care the plates can be

introduced with sufficient accuracy to make the test practical.

Footnote 56:

A scale or chart of interference colors, or the interference color

diagram, should be before the observer in order to avoid any mistakes

as to whether the new color is higher or lower in the scale.

Footnote 57:

The quartz wedge is cut so that one of its faces is exactly parallel

to the _ć_ axis (hence also parallel to the _c_ vibration direction)

while the other face makes a very small angle with it. The direction

_c_ is marked on the wedge.

Footnote 58:

Described under next test.

Footnote 59:

In applying this rule count the 1° order white as green and the 1°

order gray as blue.

Footnote 60:

A. J. Moses, _Trans. N. Y. Acad. Sci._, Vol. XVI., p. 55, Jan., 1897.

Footnote 61:

E. von Federow, _Zeit. f. Kryst., etc._, Vol. XXXV., p. 340, 1895.

Footnote 62:

After the first rough determination of the phase difference by the

mica wedge, the more exact phase difference can be obtained by the aid

of a good color chart or diagram, see end of book.

Footnote 63:

It is not safe to use minerals near the edge of the section, as the

thicknesses are apt to be unequal.

Footnote 64:

See at end of appendix.

Footnote 65:

In this way eliminate, so far as possible, the effect of the

orientation of the mineral section.

Footnote 66:

The different mineral sections are all supposed to have the same

thickness throughout the rock section.

Footnote 67:

Harker’s _Petrology for Students_, 1895, p. 14.

Footnote 68:

Iddings’ _Rock Minerals_, pp. 153, 173. Moses’ _Characters of

Crystals_, p. 115.

Footnote 69:

In the Seibert microscope use No. V objective, in Fuess microscope No.

7 objective, and in English microscopes a ¼″ or ⅕″ objective.

Footnote 70:

Each convergent ray will have its vibration direction either in or at

90° to the plane through the ray and the optic axis. Hence all rays

vibrating parallel to the vibration planes of both nicols will be

completely cut out. As the section is rotated new rays successively

come into these positions, so the same effect is maintained.

Footnote 71:

In the Seibert microscope there is a little slot _k_ for this purpose

just above the objective.

Footnote 72:

The optical character may also be determined in parallel light by

proving _ć_ = c(+), _ć_ = a(−). The optical character of the principal

zone or the sign of the elongation is often given in tables. This

optical character or sign is (+) when the principal zone axis or the

direction of elongation is parallel to c and (−) when parallel to a.

Footnote 73:

Iddings’ _Rock Minerals_, 1911, p. 172.

Footnote 74:

This assumes the optic axes for different colors to emerge about at

the same points. If there is marked “dispersion” the black bands and

hyperbolas may be rainbow-hued, as with titanite.

Footnote 75:

The interference figure, perpendicular to the _obtuse bisectrix_,

would be of the same type with a larger axial angle. Ordinarily this

figure would not come within the limits of the field of view of the

microscope. Confusion may arise, however, but in a section

perpendicular to the acute bisectrix the cross dissolves more slowly

into the hyperbolas than in the case of a section perpendicular to the

obtuse bisectrix. At times it may be necessary to measure the axial

angle to be sure. When, however, the mineral is known, the section

perpendicular to the acute bisectrix can be recognized, because if the

mineral is optically positive the trace of the axial plane is parallel

to a and if negative parallel to c.

Footnote 76:

For construction of quartz wedge, see p. 34.

Footnote 77:

The wedge can be introduced in either of the several ways described

for the introduction of the test-plates on p. 33.

Footnote 78:

For methods of measuring the axial angle, see _Methods of

Petrographic-Microscopic Research_, F. E. Wright, 1911, p. 147.

For convenience in many cases only 2_E_ is recorded, as then an

indication is given as to whether the axial angle is visible with an

ordinary microscope (arranged for observation with convergent light

for interference figures). If 2_E_ is very large the axial angle can

only be observed by covering the section with some transparent,

strongly refracting fluid. For the Seibert microscope with objective V

the limit for good results is about 2_E_ = 90°–100°.

Footnote 79:

For dispersion, etc., see A. J. Moses’ _Characters of Crystals_, p.

140.

Footnote 80:

The system of crystallization of leucite has been the subject of much

discussion. Its habit is isometric. The consensus of opinion seems to

be that leucite crystallizes in the isometric system, but that the

isometric molecular arrangement, at least of the larger crystals,

cannot exist for the temperature and pressure at the earth’s surface.

Hence molecular displacement takes place, giving rise to a more or

less complicated apparent twinning, and optical anomalies are noticed.

The isotropic character returns if the section is heated to 500° C.

Iddings’ _Rock Minerals_, p. 249, 1911.

Footnote 81:

C. W. Knight, _Canad. Rec. of Sci._, IX, No. 5. 265.

Footnote 82:

The interference colors of all minerals here recorded are those given

by sections 0.03 _mm._ in thickness (very thin sections).

Footnote 83:

Shown by Mügge, Joly, etc., to be caused by radiations emanating from

U, Th, R, etc. Iddings’ _Rock Minerals_, 1911, p. 189.

Footnote 84:

Iddings’ _Rock Minerals_, 1911, p. 392.

Footnote 85:

See page 31.

Footnote 86:

R. D. Irving, _Am. Jour. Sci._, June, 1883.

Footnote 87:

Granites of the central Alps, where the calcite crystals are

intergrown with quartz.

Footnote 88:

The minerals Nephelite, leucite, sodalite (haüynite and noselite) and

melilite are often grouped together under the name “_feldspathoides_”;

on account of their relation in rocks being equivalent to that of the

feldspars.

Footnote 89:

Oriented in conformity to the intergrowth with augite, etc., (010) and

(100) are reversed.

Footnote 90:

For other alteration processes, see Iddings’ _Rock Minerals_, p. 380.

Footnote 91:

May be difficult to determine in the case of prism zone sections,

showing large extinction angles.

Footnote 92:

See p. 88.

Footnote 93:

Iddings’ _Rock Minerals_, p. 456, 1911.

Footnote 94:

Depending on whether the axial plane is parallel or at right angles to

the clino pinacoid (010) (the plane of symmetry), we have micas of the

second (biotite) or first order (muscovite).

Footnote 95:

The distinction between zoisite α and β (essentially orthorhombic, but

may be composite triclinic twins) and clinozoisite (monoclinic close

to orthorhombic) depends on differences in position of plane of optic

axes; axial figures shown by cleavage plates; dispersion; anomalous

interference colors; etc. See Weinschenk’s _Die Gesteinbildenden

Mineralien_, p. 83. 1901.

Footnote 96:

Test not easily made on account of the very high order interference

colors, resulting from the strong double refraction.

Footnote 97:

See under quartz, p. 63.

Footnote 98:

Iddings’ _Rock Minerals_, p. 208, 1911.

Footnote 99:

On account of the weak double refraction the interference figures are

not very sharp or well defined in thin sections. In most cases only

the black hyperbolas are seen, without any colored curves.

Footnote 100:

By heating feldspar crystals the axial angle decreases to 0° and then

increases in the plane of symmetry (at right angles to its former

position). On cooling the axial angle returns to its former position

if the temperature has not exceeded 500° C. If the temperature has

been 600°–1000° C. for some time the axial angle will not return to

its former position. This fact may give some clew as to the

temperature at which the feldspar crystals formed.

Footnote 101:

This change to kaolin or clay in granite is called by Dolomieu “_La

maladie du granit_.”

Footnote 102:

See p. 31.

Footnote 103:

Hatch’s _Introduction to the Study of Petrology_, p. 33.

Footnote 104:

J. W. Judd, _Geol. Mag._ [3], Vol. VI, p. 243, 1889.

Footnote 105:

The plagioclases have rather a complex composition; but may be

regarded as forming a series from the composition NaAlSi_{3}O_{8}(Ab)

to the composition CaAl_{2}Si_{2}O_{8}(An), consisting for the most

part of isomorphous mixtures of these types, with some replacement by

KAlSi_{3}O_{8}. The compositions of only a few of the common

plagioclases are given above.

Footnote 106:

The lath-shaped feldspars, moulding the augite, give to diabases the

so-called “ophitic” structure, Fig. 12. The peculiarity of this

structure is that the feldspars crystallized before the augite, which

is contrary to the usual order of formation.

Footnote 107:

For the positions of the optic axes, bisectrices, etc., relative to

the cleavage plates of the different plagioclases, see Iddings’ _Rock

Minerals_, p. 222, 1911.

Footnote 108:

_Die Gesteinsbildenden Mineralien_ (with tables), E. Weinschenk,

Freiburg, 1901. _Étude sur la Détermination des Feldspaths dans les

Plaques Minces_, Michel Lévy, Paris, 1894; and _The Determination of

the Feldspars_, N. H. Winchell, _Am. Geol._, Vol. XXI, No. 1, 1898.

Iddings’ _Rock Minerals_, Wiley & Sons, 1911. _Étude sur la

Détermination des Feldspaths_ (troisième fascicule), Michel Lévy,

Paris, 1904.

Footnote 109:

Glass models of the feldspars (size 20 × 10 cm.) by F. Krantz, Bonn.

Diagrams, showing optical orientation in the plagioclases, in _Die

Gesteinsbildenden Mineralien_, E. Weinschenk, p. 133, 1901.

Footnote 110:

For this method of investigation little cleavage flakes or plates can

often be obtained from the crushed mineral, but, on account of Albite

twinning, plates are more apt to be obtained parallel to the twinning

plane than to the best basal cleavage. If a fragment with only one

cleavage surface is obtained, it must be cemented to a glass by this

surface and ground down to a thin section with parallel sides.

Footnote 111:

This test is only possible when suitable sections of the given

feldspar in the rock section can be found. The method, however, can be

used with great accuracy with the aid of some form of apparatus for

properly orienting the section. See “Klein’s Apparatus for the

Orientation of Thin Sections,” _Sitzungsber. Berlin. Akad._, 1895,

1151; (also in _N. Y. Acad. Sci._, Vol. XVI, p. 51, 1897); and Von

Federov’s “Universal Table,” _Zeit. für Kryst, etc._, Vol. XXV., p.

351.

Footnote 112:

In the determination of feldspar microlites it is well to remember the

following facts: “Microcline is rarely, or never, seen in the

condition of microlites, while the associations of labradorite and

albite are so different that there is little danger of confounding

them. Labradorite is the commonest product of the consolidation of the

basic eruptives, and albite almost invariably results from

metamorphism, frequently from the contact of igneous rocks on the

calcareous clastics.” N. H. Winchell, Determination of the Feldspars,

_Am. Geol._, Vol. XXI, No. 1, p. 33, 1898.

Footnote 113:

These methods (both 2 and 3) are often not applicable on account of

the tendency of the crystals in an effusive rock to parallel

orientation, which may be so marked that the rock section does not

show any favorable sections of the plagioclase.

Footnote 114:

These extinction angles, as well as those previously given, are those

of only a few type feldspars of definite composition. As the

composition varies through a long series, so the extinction angle

changes, one being a function of the other.

For a complete list of compositions and related extinction angles, see

Iddings’ _Rock Minerals_ and Lévy & Lacroix’s _Les Minéraux des

Roches_.

Footnote 115:

Iddings’ _Rock Minerals_, p. 228, Wiley & Sons, 1911. _Étude sur la

Détermination des Feldspaths_ (troisième fascicule), Michel Lévy,

Paris, 1904.

Footnote 116:

In quartz ω is the refractive index of the ray with vibration

direction ∥ a [that is the direction of vibration of the faster ray

(the ordinary ray)]. Hence ω is direction ∥ a and ε ∥ c. In the

feldspars; α ∥ a, γ ∥ c and β ∥ b.

Footnote 117:

_Am. Jour. Sci._, May, 1906. This method is specially useful in

detecting presence of orthoclase, when plagioclase is the dominant

feldspar.

Footnote 118:

These tests are only possible on pure and fresh material. The specific

gravity increases with the Ca % (albite 2.62, anorthite 2.75).

Footnote 119:

In clear unstriated granules, which may be distinguished from quartz

by biaxial interference figure in convergent light.

Footnote 120:

The tendency of labradorite in gabbros to twinning, after both

_Albite_ and _Pericline_ laws, is to be noted.

Footnote 121:

Werveke’s (N. J. B., 1883, II, 97) theory is that a twin lamination

may be caused by the forces producing mechanical deformations, as

movement in the magma and mountain making pressure. Such lamellæ are

characterized by the fact that their extent and course seem to depend

on fracture lines in the crystal.

Footnote 122:

The derivation from pyroxene and amphibole appears to be doubtful, see

Weinschenk’s _Gesteinsbildenden Mineralien_, 1901, p. 121.

Footnote 123:

Harker’s _Petrology for Students_, p. 63, 1895.

Footnote 124:

Sections can be obtained from Voight & Hochgesang, Göttingen; C.

Marchand, rue Censier, 16ter, Paris; W. H. Tomlinson, Swarthmore, Pa.,

and G. D. Julien, 3 Webster Terrace, New Rochelle, N. Y.

Footnote 125:

Made by G. D. Julien, 3 Webster Terrace, New Rochelle, N. Y. Price:

Power lathes (complete), $150.00 up; Foot-treadle lathes, $90.00 up.

Footnote 126:

A Crocker-Wheeler motor of ¼ to ½ H. P. will be large enough for an

ordinary laboratory machine.

Footnote 127:

Made by Voigt and Hochgesang, Göttingen. Price, $15.00.

Footnote 128:

Saws charged with diamond dust can be obtained from Elisha T. Jenks,

Middleboro, Mass. Price in 1910, $1.35 per diametrical inch. Foreign

saws 6″ and 8″ diam. can be bought from G. D. Julien, New Rochelle, N.

Y.

Footnote 129:

_School of Mines Quarterly_, Vol. XI, p. 32.

Footnote 130:

“Half a pound or less of ordinary shellac is melted in a flat-bottomed

open vessel over a Bunsen burner. Then an equal quantity of Venice

turpentine is carefully added under constant stirring. The mass should

be allowed to boil for about ten minutes, during which the stirring is

continued. Then small quantities are poured in separate heaps on an

iron plate or other cold surface and rolled into sticks about seven

inches long and half an inch thick.”

Footnote 131:

Square or standard 26 × 46 mm. glass slides are recommended instead of

the oblong slides (1 × 3 inches), which are very apt to project beyond

the edges of the stage and be struck by the fingers while rotating the

stage.

Footnote 132:

Reference can be made to the publications on this subject by: Borichy,

Behrens (Behren’s translation by Judd), Haushofer, Huysse, Klément,

Streng, Rénard, etc.

Footnote 133:

In case an acid is to be used which would attack glass, the

cover-glass can be replaced by a thin perforated disk of platinum.

Footnote 134:

The bases in solution can be determined by different methods of

analysis, for which the student is referred to more elaborate works on

this subject. In some cases it may be very advantageous to treat the

section with acid, to remove certain soluble constituents, when other

minerals not distinctly seen at first may be made more apparent.

Footnote 135:

The gas may be H_{2}S from a soluble sulphide, in which case the

solution containing the bubbles will color filter paper moistened with

lead water.

Footnote 136:

_Geol. and Nat. History Survey of Minn._, XIX., Ann. Rept., p. 42;

also A. J. Moses, _Characters of Crystals_, p. 147.

Footnote 137:

The symmetry of the etched figures would, of course, be related to the

system of crystallization.

Footnote 138:

A. J. Moses, _Characters of Crystals_, Chap. XVI.

Footnote 139:

When it is desired to preserve the section and at the same time to

study the surface covered with a film of air, the edges alone of the

cover-glass should be cemented.

Footnote 140:

_Geol. and Nat. Hist. Survey of Minn._, XIX, Ann. Rept., p. 50. Thin

sections of 2–3 sq. mm. area are of a convenient size, and they should

be subjected to a red heat for (1½)-3 minutes. Too long a continuance

of heat may render the sections too dark or lessen their transparency

or produce melting.

Footnote 141:

This test may vary, in many cases graphite not being consumed even

after long heating.

Footnote 142:

The isolation of material for investigation is of more interest for

the lithologist or chemist than for the student of optical mineralogy;

therefore only a very brief outline of some of the methods employed

will be given.

Footnote 143:

The grains passing through different meshes are investigated

microscopically to ascertain which size grains are homogeneous; the

rest of the sample should then be reduced to grains of this size.

Footnote 144:

Further reference can be made to _Iddings’ Rock Minerals_, pp. 25 and

95, 1911. A convenient form of apparatus is also described in _School

of Mines Quarterly_, Vol. X., p. 284, 1889.

Footnote 145:

S. L. Penfield, _Am. Jour. Sci._, Vol. L., p. 446, 1895. In this

article a convenient form of separating apparatus is also described.

Footnote 146:

A convenient list of minerals, arranged in the order in which they

would be attracted by increasing the force of the electro-magnet, is

given in Weinschenk’s _Tabellen_.

Footnote 147:

For micro-chemical work the reagents should be applied in very small

drops, which spread out on glass to discs 2 mm. in diameter. For

manipulating the reagents use platinum wires, 0.5 mm. in thickness.

Footnote 148:

_Elemente einer neuen chemisch-mikroskopischen mineral- und

Gesteins-analyse_, Pragg, 1877.

Translation of above by Winchell in _Geol. and Nat. Hist. Survey of

Minn._, Vol. XIX., Ann. Report, 1890.

Footnote 149:

The strength of the solution should be about 3½%; for if too weak many

minerals do not give satisfactory results, and if too strong a very

large number of fluosilicate crystals are formed together with the

separation of much silica, thus making it impossible to carefully

differentiate the crystals with a microscope.

Footnote 150:

As most of the rock-forming minerals that would be investigated are

silicates, the hydrofluosilicic solutions can also be obtained by

treatment with HFl.

Footnote 151:

After Lévy and Lacroix.

Footnote 152:

_Naturkunde_, Amsterdam, 2, Vol. XVII., 1881. _Chemical News_, Vol.

LXIII., No. 1647, June 1891, et seq.

_Micro-chemical Analysis_, Behrens (Judd), Macmillan & Co., London,

1894.

Footnote 153:

After Lévy and Lacroix.

Footnote 154:

After Lévy and Lacroix.

Footnote 155:

Compiled from Weinschenk’s Tables, as revised in _Petrographic

Methods_ by Weinschenk-Clark, 1912.

Footnote 156:

Pirsson and Robinson, _Am. Jour. Sci._, iv, Vol. X, Oct., 1900.

Footnote 157:

Harker, _Petrology for Students_, p. 28, 1895.

Footnote 158:

Have the convergent lens or condenser lowered and the analyzer out

during this test.

Footnote 159:

The minerals are grouped according to the maximum interference colors

given by sections of the thickness of 0.03 mm.

Footnote 160:

In the case of very small crystals, the centering must be accurate and

a cover with a small hole in the center, should be placed over the top

of the tube. In this way the eye is brought directly over the axis of

the microscope and figures can be observed from very minute crystals.

------------------------------------------------------------------------

TRANSCRIBER’S NOTES

Page Changed from Changed to

80 occurs as an alternation product occurs as an alteration product

of anhydrite. Gypsum is soluble of anhydrite. Gypsum is soluble

in hydrochloric in hydrochloric

136 longer the higher the percentage longer the higher the percentage

of calcium in the solution of sodium in the solution

● Typos fixed; non-standard spelling and dialect retained.

● The author used the old chemical symbol (Fl) for Fluorine.

● Corrected the Errata with the exception of the last paragraph

"Corrections for mean indices of refraction in Scheme (insert

folder)".

● Used numbers for footnotes, placing them all at the end of the last

chapter.

● Enclosed italics font in _underscores_.

● Enclosed bold font in ▄lower half block▄.

● The caret (^) serves as a superscript indicator, applicable to

individual characters (like 2^d) and even entire phrases (like

1^{st}).

● Subscripts are shown using an underscore (_) with curly braces { },

as in H_{2}O.