TABLE 3.--TESTS OF "HIDALGO" CEMENT WITH VARIOUS SANDS.

=====================================+============+============

Sand. | At 7 days. | At 28 days.

-------------------------------------+------------+------------

Ottawa (Standard) | 305 lb. | 414 lb.

Monterrey, 1-1/2 parts, } | |

Hornos, 1-1/2 parts } | 188 " | 313 "

Monterrey | 253 " | 365 "

Hornos | 202 " | 301 "

Manufactured sand, Company's crusher | 372 " | 566 "

Hornos, 2 parts, } | |

Crusher sand, 1 part } | 231 " | 352 "

Hornos, 1-1/2 parts, } | |

Crusher sand, 1-1/2 parts } | 265 " | 346 "

Hornos, 1 part, } | |

Crusher sand, 2 parts } | 248 " | 328 "

=====================================+============+============

The Hornos sand was used during a few weeks in the latter part of 1908,

when the crusher was unable to produce all that was required. Its use

was restricted to thick walls which were required to be water-tight, and

it was always used in equal proportions with the crusher dust.

ASCE 1193: The Water-Works and Sewerage of Monterrey, N. L., Mexico The 4th article from the June, 1911, Volume LXXII, Transactions of the American Society of Civil Engineers. Paper No. 1193, Feb. 1, 1911. · 第 16 / 48 题