CHAPTER III.

MORDANTS

Definition of mordant. The principal mordants. The

mordanting of silk and wool. Of linen and cotton.

Astringents for cotton. Alum. Various examples of using

alum for wool, silk, cotton and linen. Iron. Examples of

iron mordants. Tin. Examples of tin mordants. Chrome.

Examples of chrome mordants. Copper. Examples of copper

mordants. General observations. Tannin and the galling of

cotton and linen. Examples of various galling processes.

MORDANTS.--Dyes are divided into two classes. First, the _substantive_

dyes, which give their colour directly to the material with which they

are boiled: and second, the _adjective_ dyes, as they are sometimes

called. These latter include the greater number of dyes and require

the use of a mordant to bring out their colour.

There are thus two processes concerned with the dyeing of most

colours; the first is mordanting and the second is the colouring or

actual dyeing. The mordanting prepares the stuff to receive the

dye--(_mordere_, to bite.) The early French dyers thought that a

mordant had the effect of opening the pores of the fibres, so that the

dye could more easily enter; but according to Hummel and later dyers

the action of the mordant is purely chemical; and he gives a

definition of a mordant as "that body, whatever it may be, which is

fixed on the fibre in combination with any given colouring matter."

The mordant is first precipitated on to the fibre and combines with

the colouring matter in the subsequent dye bath. But, whether the

action is chemical or merely physical, the fact remains that all

adjective dyes need this preparation of the fibre before they will fix

themselves on it. The use of a mordant, though not a necessity, is

sometimes an advantage when using substantive dyes.

In early days the leaves and roots of certain plants were used. This

is the case even now in India and other parts where primitive dyeing

methods are still carried on. Alum has been known for centuries in

Europe. Iron and tin filings have also been used. Alum and copperas

have been known in the Highlands for long ages. Stale urine is also

much used in Scotland and Ireland, but perhaps more as a clearing

agent than as an actual mordant.

Silk and wool require very much the same preparation except that in

the case of silk high temperatures should be avoided. Wool is

generally boiled in a weak solution of whatever mordant is used. With

silk, as a rule, it is better to use a cold solution, or a solution at

a temperature below boiling point. Cotton and linen are more difficult

to dye than wool or silk. Their fibre is not so porous and will not

hold the dye stuff without a more complicated preparation. The usual

method of preparing linen or cotton is to boil it first with some

astringent. The use of astringents in dyeing depends upon the tannic

acid they contain. In combination with ordinary mordants, tannic acid

aids the attraction of the colouring matter to the fibre and adds

brilliancy to the colours. The astringents mostly used are tannic

acid, gall nuts, sumach and myrobalams. Cotton has a natural

attraction for tannic acid, so that when once steeped in its solution

it is not easily removed by washing.

ALUM. (_Aluminium sulphate._)--This is the most generally used of all

the mordants, and has been known as such from early times in many

parts of the world. For most colours a certain proportion of cream of

tartar should be added to the alum bath as it helps to brighten the

ultimate colour. The usual amount of alum used is a quarter of a pound

to every pound of wool. As a rule, less mordant is needed for light

colours than for dark. An excess of alum is apt to make the wool

sticky.

"For dyeing worsted and stuffs yellow, you make use of the usual

preparation, viz., of tartar and alum. You allow four ounces of alum

to every pound of wool, or twenty-five pounds to every hundred. With

regard to the tartar, one ounce to every pound is sufficient for

yellow, though it requires two for red."--Hellot.

The usual length of time for boiling with alum is from ½ an hour to 1

hour; but some dyers give as much as 2½ hours.

_Various examples of mordanting with alum._--

_For silk._ Wet out the silk thoroughly with water and wring out. Then

work it about a little in a strong solution of alum, previously

dissolved in hot water, and steep for several hours (or over night).

Then wash well. It should not be allowed to dry before dyeing. "Silks

are always alumed in the cold, because when they are alumed in a hot

bath, they are apt to lose a portion of their lustre." _Berthollet._

_For wool._ ¼ lb. of Alum and 1 oz. Cream of tartar for every pound of

wool. This is dissolved and when the water is warm the wool is

entered. Raise to boiling point and boil for one hour. The bath is

then taken off the fire and allowed to cool over night. The wool is

then wrung out (not washed) and put away in a linen bag in cool place

for four or five days, when it is ready for dyeing.

_For cotton and linen._ After boiling in water (some use a sour water,

some an alkaline ley) the cotton is put into the alum bath, ¼ lb. of

Alum to 1 lb. of cotton. The alum is dissolved in hot water with soda

in the proportion of 1 part soda to 16 of alum. (Some add a small

quantity of tartar and arsenic). The cotton is well worked in this

solution and left 24 hours. It is then washed, and afterwards galled.

_For linen._ ¼ lb. alum for every pound of linen. Boil for 2½ hours

and immediately put into the dye bath.

_For wool._ 6 to 8 per cent. of alum and 5 to 7 per cent. of tartar of

the weight of wool.

IRON. (_Ferrous Sulphate_, _copperas_, _green vitriol_)

Iron is one of the oldest mordants known and is largely used in wool

and cotton dyeing. It is almost as important as alum. With wool it

should be used in combination with cream of tartar. The temperature of

the mordanting bath must be raised very gradually to boiling point or

the wool will dye unevenly. A general method of dealing with copperas

is to boil the wool first in a decoction of the colouring matter and

then add the mordant to the same bath in a proportion of 5 to 8 per

cent. of the weight of wool: and continue boiling for half an hour or

so longer. With some dyes a separate bath is needed, such as with

Camwood or Catechu. If used for cotton, the cotton is first dyed in a

boiling decoction of the dye stuff and then passed through a cold

solution of ferrous sulphate. Probably the commonest way of applying

copperas in cotton dyeing is to prepare the cotton with tannin, pass

through clear lime water and then through a copperas solution. Great

care is needed in the using of copperas, as, unless it is thoroughly

dissolved and mixed with the water before the wool is entered, it is

apt to stain the wool. It also hardens wool if used in excess, or if

boiled too long.

Copperas is mostly used for the fixing of wool colours (Fustic etc.)

to produce brown shades by the "stuffing and saddening" method (see

page 14), the wool being boiled first in a decoction of the dye for

about an hour, and then for ½ an hour with the addition of 5 to 8 per

cent. of copperas. If used for darkening colours, copperas is added to

the bath, after the dyeing, and the boiling continued for 15 to 20

minutes.

_Examples of various proportions for Mordanting._--

8 per cent. of copperas and 20 per cent. of cream of tartar is a

mordant used for some colours.

4 per cent. copperas, 10 per cent. cream of tartar gives good olive

colours with weld.

8 per cent. copperas without tartar with single bath method, for dark

olive brown with old fustic.

2 oz. copperas and 2 oz. cream of tartar to 2½ lbs. wool.

2 oz. copperas, 1½ oz. oxalic acid to 2½ lbs. wool.

TIN.--(_Stannous chloride_, _tin crystals_, _tin salts_, _muriate of

tin_.)

Tin is not so useful as a mordant in itself, but as a modifying agent

with other mordants. It must be always used with great care, as it

tends to harden the wool, making it harsh and brittle. Its general

effect is to give brighter, clearer and faster colours than the other

mordants. When used as a mordant before dyeing, the wool is entered

into the cold mordanting bath, containing 4 per cent. of stannous

chloride and 2 per cent. oxalic acid: the temperature is gradually

raised to boiling, and kept at this temperature for 1 hour. It is

sometimes added to the dye bath towards the end of dyeing, to

intensify and brighten the colour. It is also used with cochineal for

scarlet on wool, in the proportion of 6 per cent. of stannous chloride

and 4 per cent. of cream of tartar. Boil for 1 to 1½ hours. Then wash

well. The washing after mordanting is not always essential. Also 6 to

8 per cent. of oxalic acid and 6 per cent. of stannous chloride, for

cochineal on wool. This mordant produces bright fast yellows from old

fustic, by boiling the wool from 1 to 1¼ hours, with 8 per cent. of

stannous chloride and 8 per cent. of cream of tartar. One recipe

gives 2 oz. tin and 4¼ oz. cream of tartar to 2½ lbs. wool in 10

gallons of water. It is not a suitable mordant alone for cotton, but

can be used to brighten the colour in combination with other mordants.

"The nitro-muriate of tin (dyer's spirit) although it produces good

yellows with quercitron bark, produces them in a much weaker degree

than the murio-sulphate of that metal, which is really the cheapest

and most efficacious of all the solutions or preparations of tin for

dyeing quercitron as well as the cochineal colours."-- _Bancroft._

CHROME. (_Potassium dichromate_, _Bichromate of Potash._)

Chrome is a modern mordant, unknown to the dyer of 50 years ago. It is

excellent for wool and is easy to use and very effective in its

action. Its great advantage is that it leaves the wool soft to the

touch, whereas the other mordants are apt to harden the wool. In

commercial dyeing it is now almost exclusively used, as it has proved

itself the most generally convenient. By some it is said not to be so

fast to light as the other mordants, but it produces brighter colours.

The wool should be boiled for one to one & a half hours with

bichromate of potash in the proportion of 2 to 4 per cent. of the

wool. It is then washed well and immediately dyed. Wool mordanted with

chrome should not be exposed to light, but should be kept well covered

with the liquid while being mordanted, else it is liable to dye

unevenly. An excess of chrome impairs the colour. 3 per cent. of

chrome is a safe quantity to use for ordinary dyeing. One recipe gives

1½ oz. of chrome to 2½ lbs. of wool. It should be dissolved in the

bath while the water is heating. The wool is entered and the bath

gradually raised to the boiling point, and boiled for three quarters

of an hour.

In the dyeing of cotton, it is used for catechu browns and other

colours. The cotton is soaked in a decoction of catechu, and

afterwards passed through a boiling solution of chrome, or it is

worked for half an hour in a bath of chrome at 60°C., and then washed.

It is usual to wash wool or cotton after mordanting with chrome, but

some dyers do not think it necessary.

COPPER. (_Copper Sulphate_, _Verdigris_, _blue vitriol_,

_blue-stone_.)

Copper is rarely used as a mordant. It is usually applied as a

saddening agent, that is, the wool is dyed first, and the mordant

applied afterwards to fix the colour. With cream of tartar it is used

sometimes as an ordinary mordant before dyeing, but the colours so

produced have no advantage over colours mordanted by easier methods\.

EXAMPLES.--6 per cent. of copper is used as a mordant for weld to

produce an olive yellow. 4 to 5 per cent. is used with old fustic for

yellow. 10 per cent. of copper gives to wool a reddish purple with

cochineal.

Mordants should not affect the physical characteristics of the fibres.

Sufficient time must be allowed for the mordant to penetrate the fibre

thoroughly. If the mordant is only superficial, the dye will be

uneven: it will fade and will not be as brilliant as it should be. The

brilliancy and fastness of Eastern dyes are probably due to a great

extent to the length of time taken over the various processes of

dyeing. _The longer time that can be given to each process, the more

satisfactory will be the result._

Different mordants give different colours with the same dye stuff. For

example:--Cochineal, if mordanted with alum, will give a crimson

colour; with iron, purple; with tin, scarlet; and with chrome or

copper, purple. Logwood, also, if mordanted with alum, gives a mauve

colour; if mordanted with chrome, it gives a blue. Fustic, weld, and

most of the yellow dyes, give a greeny yellow with alum, but an old

gold colour with chrome; and fawns of various shades with other

mordants.

TANNIN.--(_Tannic Acid_.)--Tannins are used in the dyeing of cotton

and linen. Cotton and linen possess the remarkable power of attracting

tannins from their aqueous solution, and when these substances are

prepared with tannins, they are able to retain dyes permanently.

Cotton saturated with tannin, attracts the dye stuff more rapidly, and

holds it. Tannic acid is the best tannin for mordanting cotton and

linen, as it is the purest and is free from any other colouring

matter. It is, therefore, used for pale and bright shades. But for

dark shades, substances containing tannic acid are used, such as

sumach, myrobalans, valonia, divi-divi, oak galls, chestnut (8 to 10

per cent. of tannin), catechu.

Cotton and linen are prepared with tannin after they have been through

the required cleansing, and if necessary, bleaching operations. A

bath is prepared with 2 to 5 per cent. of tannic acid of the weight of

the cotton, and a sufficient quantity of water. For dark shades, 5 to

10 per cent. should be used. The bath is used either hot or cold. It

should not be above 60°C. The cotton is worked in this for some time,

and then left to soak for 3 to 12 hours, while the bath cools. It is

then wrung out and slightly washed.

The following gives the relative proportions of the various substances

containing tannin:--1 lb. tannin _equals_ 4 lbs. sumach, 18 lbs.

myrobalans, 14 lbs. divi-divi, 11 lbs. oak galls.

A few examples taken from various recipes of cotton dyeing:--

For 10 lbs. cotton use 12 oz. tannin.

For 50 lbs. cotton use 10 lbs. sumach.

For 40 lbs. cotton use 10 lbs. sumach.

For 20 lbs. cotton use 2 lbs. yellow catechu or black catechu.

For 20 lbs cotton spend 3 lbs. of catechu with 3 oz. of blue

vitriol.

Some recipes soak the cotton for 24 hours, others for 48 hours.

A Book on Vegetable Dyes · 第 3 / 10 章